Home 中文
Stainless steel tubes used for pressure
Standard:EN10216-5
Size:OD(6-508mm)×WT(0.5-25mm)
Material: 1.4301, 1.4306, 1.4401, 1.4404, 1.4410, 1.4462 and so on
Application:The stainless steel seamless tubes for pressure purposes

Chemical composition of austenitic corrosion-resistant steel

Grade

Cmax

Si

Mn

Pmax

Smax

N

Cr

Cu

Mo

Ni

Ti

1.4307

0.03

≤1

≤2

0.04

0.015b

≤0.11

17.5-19.5

-

-

8.0-10.0c

-

1.4306

0.03

≤1

≤2

0.04

0.015b

≤0.11

18.0-20.0

-

-

10.0-12.0d

-

1.4301

0.07

≤1

≤2

0.04

0.015 b

≤0.11

17.0-19.5

-

-

8.0-10.5

-

1.4541

0.08

≤1

≤2

0.04

0.015

-

17.0-19.0

-

-

9.0-12.0d

5xC-0.70

1.4550

0.08

≤1

≤2

0.04

0.015

-

17.0-19.0

-

-

9.0-12.0d

-

1.4335

0.02

≤0

≤2

0.025

0.01

≤0.11

24.0-26.0

-

≤0.20

20.0-22.0

-

1.4404

0.03

≤1

≤2

0.04

0.015 b

≤0.11

16.5-18.5

-

2.0-2.5

10.0-13.0e

-

1.4401

0.07

≤1

≤2

0.04

0.015 b

≤0.11

16.5-18.5

-

2.0-2.5

10.0-13.0

-

1.4571

0.08

≤1

≤2

0.04

0.015 b

-

16.5-18.5

-

2.0-2.5

10.5-13.5c

5xC-0.70

1.4436

0.05

≤1

≤2

0.04

0.015 b

≤0.11

16.5-18.5

-

2.0-3.0

10.5-13.0d

-

1.4435

0.03

≤1

≤2

0.04

0.015 b

≤0.11

17.0-19.0

-

2.0-3.0

12.5-15.0

-

1.4539

0.02

≤0.7

≤2

0.03

0.01

≤0.15

19.0-21.0

1.2-2

4.0-5.0

24.0-26.0

-

 

 Chemical composition of austenitic creep-resistant steel 

Grade

Cmax

Si

Mn

Pmax

Smax

N

Cr

Mo

Nb

Ni

1.4948

0.04-0.08

≤1.00

≤2

0.035

0.015

≤0.11

17-19

-

-

8-11

1.4940

0.04-0.08

≤1.00

≤2

0.04

0.015

≤0.11

17-19

-

-

9-13

1.4912

0.04-0.10

≤1.00

≤2

0.04

0.015

≤0.11

17-19

-

10xC-1.2

9-12

1.4918

0.04-0.08

≤0.75

≤2

0.035

0.015

≤0.11

16-18

2.0-2.5

 

12-14

 

 Chemical composition of duplex stainless steel

Grade

Cmax

Si

Mn

Pmax

Smax

N

Cr

Cu

Mo

Ni

1.4462

0.03

≤1.0

≤2.0

0.035

0.015

0.1-0.22

21-23

-

2.5-3.5

4.5-6.5

1.4362

0.03

≤1.0

≤2.0

0.035

0.015

0.05-0.2

22-24

0.1-0.6

0.1-0.6

3.5-5.5

1.4410

0.03

≤1.0

≤2.0

0.035

0.015

0.2-0.35

24-26

-

3-4.5

6.0-8.0

1.4507

0.03

≤0.7

≤2.0

0.035

0.015

0.15-0.3

24-26

1-2.5

2.7-4

5.5-7.5

1.4501

0.03

≤1.0

≤1.0

0.035

0.015

0.2-0.3

24-26

0.5-1

3-4

6.0-8.0

 

Mechanical properties of corrosion-resistant austenitic steel

Mechanical properties

Yield strength, min, Mpa

Tensile strength

Elongation min%

Impact properties, min, KV/J

Room temperature

0-196

Grade

Rp0.2

Rp1.0

Rm, Mpa

1

t

1

t

t

1.4307

180

215

460-680

40

35

100

60

60

1.4306

180

215

460-680

40

35

100

60

60

1.4301

195

230

500-700

40

35

100

60

60

1.4541L

200

235

500-730

35

30

100

60

60

1.4541R

180

215

460-680

35

30

100

60

60

1.4550

205

240

510-740

35

30

100

60

60

1.4335

180

210

470-670

45

40

100

60

60

1.4404

190

225

490-690

40

30

100

60

60

1.4401

205

240

510-710

40

30

100

60

60

1.4571L

210

245

500-730

35

30

100

60

-

1.4571R

190

225

490-690

35

30

100

60

60

1.4436

205

240

510-710

40

30

100

60

60

1.4435

190

225

490-690

40

30

100

60

60

1.4539

230

250

520-720

35

30

120

90

60

 

 Mechanical properties of creep resistance of austenitic steel

Mechanical properties

Yield strength, min, Mpa

Tensile strength

Elongation ,min%

Impact properties, min, KV/J

Grade

Rp0.2

Rp1.0

Rm, Mpa

1

t

1

t

1.4948

185

225

500-700

40

30

100

60

1.4940

190

220

510-710

35

30

100

60

1.4912

205

240

510-710

40

30

100

60

1.4918

205

245

490-690

35

30

100

60

 

 Mechanical properties of duplex stainless steel

Mechanical properties

Yield strength, min, Mpa

Tensile strength

Elongation ,min%

Impact properties, min, KV/J

Room temperature

0-40

Grade

Rp0.2

Rm, Mpa

1

t

1

t

t

1.4462

450

640to880f

22

22

120

90

40

1.4362

400

600to820

25

25

120

90

40

1.4410

550

800to1000

20

20

100

100

40

1.4507

500

700to900

20

20

100

100

40

1.4501

550

800to1000

20

20

100

100

40

© 2009 Shanghai Vastar International Co., Ltd 沪ICP备09068916号-1